    I am trying to improve my Mig skills and would like your help.

    Welds were done with the I mig 205 Arc force off (turned full left) .035 70s6 solid wire, 75/25 Argon Co2 gas, on 1.8 mild steel that actually Miced .115

    Welds are numbered top to bottom.

    #1 18.5 V. 140A Push
    #2 18.5 V. 140A Pull
    #3 19v 140A Push
    #4 19v 140A Pull
    #5 19v 150A Push
    #6 19 v 150A Pull

    Click image for larger version. 

Name:	205 welds 002.jpg 
Views:	614 
Size:	97.4 KB 
ID:	3132

    I am looking for input on travel speed. gun control, stick-out etc. Really anything you see that I need to work on.
    Thanks
    Ray

  2. #2

    Default

    No such a thing as off. Its all relative...more inductance, less inductance.
    It looks like it may more inductance...Orientation of high inductance position, may have changed since original units were produced.Push always with mig, unless you can't because of position.

    Travel speed is very inconsistent. Prop/ brace yourself on the metal or table, hold the gun with both hands, and move from the elbow to start.
    Looks like you may be holding torch too far off. Bring it down to 1/2" off metal.

    #5, last half is the best.
    Last edited by performance; 08-18-2011 at 08:18 PM.

  3. #3

    Default

    Hi Ray, nothing wrong with the heat/volt settings etc, just need to move faster and try to make flatter weld deposits. I would suggest practise doing laps joints as they tend to slow the whole thing down a bit and give you a bit more time to adjust to the speed of travel. consistant travel speed makes for better lookig welds.

  4. #4

    Default more welds

    I did a butt weld that I stress tested in my vice with a BFH and it held I also tried a lap weld.
    Settings were the same


    Click image for larger version. 

Name:	butt and lap welds 004.jpg 
Views:	585 
Size:	144.1 KB 
ID:	3142
    Lap weld

    Click image for larger version. 

Name:	butt and lap welds 003.jpg 
Views:	579 
Size:	145.9 KB 
ID:	3140
    Same Lap weld

    Click image for larger version. 

Name:	butt and lap welds 002.jpg 
Views:	578 
Size:	141.5 KB 
ID:	3141
    Butt weld

    Click image for larger version. 

Name:	butt and lap welds 001.jpg 
Views:	569 
Size:	79.1 KB 
ID:	3144
    Same butt weld.

  5. #5

    Default

    Ya still need to work on the travel speed. If you're right handed, try tilting your torch to the 2 o'clock position and weld right to left using a tight looping motion as you move smoothly and constantly to the left. Pause for a second at the end of your weld.
    Make a few dry runs on the piece you're going to weld before pulling the trigger and finally making the weld. Practice makes perfect.
    2013 250EX : SSC Pedal : I-MIG 250P 20' Profax gun : Power Plasma 60 p80 torch : 3M Speedglas 9100XX : Evolution Rage 3 DB cold saw

  6. #6
    Join Date
    Mar 2011
    Location
    The Boonies of Texas
    Posts
    420

    Default

    Go over to weldingtipsandtricks.com and watch some of Jody's MIG videos. It certainly helped me a lot.

    Thurmond
    Miller Bobcat 3 Phase,
    Miller Suitcase X-Treme 12VS wire feeder for the Bobcat with M-25 300A .045" gun / Bernard 400A 5/64" wire mig gun .
    26 series gas cooled TIG torch, setup for quick connect to Bobcat.
    17 series gas cooled Tig Torch for Low Amp Solar Tig (Direct Solar Panel Powered Tig welding)
    Hobart Handler 187 Mig / Fluxcore
    EVERLAST PowerUltra 205P
    EVERLAST PowerTig 250 EXT 2013 Model

  7. #7

    Default

    Ray,

    The heat and all look fine, but you are still real unsteady and inconsistent in your movement. I see a hint of too much standoff.

  8. #8
    Join Date
    Aug 2011
    Location
    South Carolina
    Posts
    9
    Blog Entries
    1

    Default

    I am new to welding and received the most helpful information as well as much practice by taking a continuing education class for MIG welding at our local Tech education center. As a senior, sight was my biggest issue. I invested in an auto dark helment and added a magnifying lens to see better. What a difference it made being able to better see the weld puddle, travel line and tourch angle.

  9. #9

    Default

    With the metal thickness that you are using I would suggest using .030 wire or less. Your running just slightly cold for the size of wire but its to hot for the the thickness of plate, see your number 6 bead. The brown around it is an indicator. Also, you need to brace yourself, use both hands, and may need to add a cheater lenses to your hood, and adjust the shade setting to where you see the puddle the best.. Watch the stickout, leave it about 3/8" to 1/2". Gas should be set 10 to 15 cfh. Play with the gas and see what works best. Pushing and moving quicker will allow the bead to flatten some if your angle of your torch is correct. You may also use a scribe line that will allow you to follow a straighter line.
    Risk Control Consultant, Boiler and Machinery
    Boiler and Pressure Vessel inspector-National Board Commission
    Simadre 520D 3n1 Plasma, DC Stick, DC TIG
    Marquette AC/DC Stick welder
    King Drill press
    DeWalt chop saws
    Shop air compressors
    Oxy/Acet. torches
    Oliver and MM tractors
    All kinds of power tools

  10. #10

    Default

    Good video on adjusting wire speed and amperage......http://www.youtube.com/watch?v=6eB9qnktmDI

    Looks like you are just going in a straight line. After making adjustments to your wire speed and amps, try making cursive e's with your gun going back a little on the previous weld area. It will make your welds a bit stronger and make it look more like a tig weld.

    Another good place to learn about mig welding is if you google "Mig like Tig". They have lots of information on how to make your mig welding strong and make them look like a tig weld.

  11. #11

    Default

    Quote Originally Posted by thinman100 View Post
    I am new to welding and received the most helpful information as well as much practice by taking a continuing education class for MIG welding at our local Tech education center. As a senior, sight was my biggest issue. I invested in an auto dark helment and added a magnifying lens to see better. What a difference it made being able to better see the weld puddle, travel line and tourch angle.
    Seeing is half the battle! When I was in welding school I started out wearing dark glasses and a #12 welding lens, together was probably a #15. I was having trouble, I was told that some people need to wear dark glasses because of welding flash from people around them, and someone told me I need to loose the glasses for regular safety glasses and get a lighter lens so I could see. I find a #10 works for me, but sometimes I go darker if I am tig welding. I could not see the puddle that was keeping me from being able to run a good bead.
    Lincoln Eagle Engine Drive
    Everlast MTS 250
    Everlast Power Tig 225lx
    HTP Mig 2400
    Everlast Power Plasma 60C --> Just need to finish my CNC Plasma Table!
    Miller Spectrum 375 Extreme Plasma cutter
    Victor cutting torch
    HF 20 Ton Shop Press
    HF 4x6 Band Saw
    HF Air Compressor
    Northern Tool Drill Press


    www.murphywelding.com

  12. #12

    Default

    They ALL look good to me lol
    Benjamin

    Owner of IMIG 200 and half owner of Power Plasma 50

    https://www.facebook.com/BenjaminRootPhotography

Similar Threads

  1. Please critique these beads
    By JohnT in forum TIG Welding (GTAW/GTAW-P)
    Replies: 5
    Last Post: 07-31-2014, 08:11 PM
  2. A few of my first welds with the I-MIG 200.....
    By CGCINC in forum MIG Welding (GMAW/GMAW-P/FCAW)
    Replies: 26
    Last Post: 04-23-2012, 03:46 PM
  3. My Welds
    By Oxide00 in forum Other Custom Fabrications
    Replies: 35
    Last Post: 11-09-2011, 11:23 AM
  4. how are my welds
    By dgarnier in forum TIG Welding (GTAW/GTAW-P)
    Replies: 26
    Last Post: 05-20-2011, 01:46 AM
  5. Weld Critique Plz
    By Haywire in forum Stick Welding (SMAW)
    Replies: 6
    Last Post: 05-06-2011, 08:53 AM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •