 Originally Posted by 
performance
					 
				 
				I think Ray may have misunderstood.
The plasma side is separate...so...
At 25 amps, you have an issue with having too large of a nozzle and too much air.  The arc is blowing out. 
If you need to operate under 40 amps, you'll need to drop nozzle sizes.   Unfortunately we do not carry the really smaller sizes, but they are out there.
75 is a wee bit much anyway as that is the MAX air pressure at max amps, actually 2.5 lbs over recommended max.  Try 50, then 60 then 65 to see if it improves, though that isn't a fix, it's just a get by until you can get a smaller nozzle.  Is the squeal coming from the torch or from the unit itself?  Some inverters have a characteristic whine to them.  In fact inverters like these with a certain switching speed are called "screamers".  It can vary a little from machine to machine, especially when new.  If its from the torch, then I have heard that too.  Have you changed out the consumable itself?  Make sure the swirl ring is firmly seated and centered.
This unit WILL NOT weld 6010.  Never has, never will, never promised. In fact we have made many forum posts about the lack of 6010 capability with these machines.  The arc will go out!  It will not be stable. 6011 is better though.  Try some 6013 or 7018.
			
		 
	 
 Mark, thanks for the quick response I will try the settings you recommended when I get to class tomorrow night. So are the nozzles that came with it the wrong size to be using? I have not changed the consumable yet as it still looks brand new.The squeal comes from the machine when the trigger is pulled and the arc does not start. Not real sure if it does it all the time due to noise of cutting. As far as the 6010 I must have misread I thought is said 6010 and 6011 but I checked again and it says 6011 only. I think we have some 6013 in class so I will try that also. Again thanks for your help and I will post my results as soon as I can.
Thanks,
Putz
				
			 
			
		 
			
			
			
				
					Last edited by putz; 01-22-2014 at 05:07 AM.
				
				
			
			
			
				
			
			