Share
Results 1 to 5 of 5

Thread: Prepping aluminum for TIG welding

Hybrid View

Previous Post Previous Post   Next Post Next Post
  1. #1
    Join Date
    Oct 2010
    Location
    Northern Virginia
    Posts
    1,323

    Default Prepping aluminum for TIG welding

    In another post, JohnT mentioned he thought the AC portion of the aluminum TIG arc would clean the aluminum. I also harbored that same thought-so my question is, when we see example welds on videos at WT&T, for instance, the explanation of AC balance makes it a point to show the frosty cathodic cleaning zone. What is the difference between those welds, which break up the aluminum oxide layer and produce the frosty clean zone, and my welds, where I have to use a flap disk to get to bare metal? Is it the alloy of aluminum, or maybe the amount of oxide that has built up?
    DaveO
    Oxweld oxy acet gear
    IMIG 200
    PowerTIG 210 EXT... Amazing!

  2. Default

    For best strength the metal should be cleaned. That said the longer the aluminum is exposed to humidity, chemicals, and air the thicker the oxide layer becomes. On new alum. the layer can be cleaned to an acceptable amount by the cleaning action of the arc but for top strength it is good to clean it anyway.
    Miller 302 gas drive
    millermatic 200 mig
    miller spoolmatic 3 spool gun with 100ft ext.
    2014 Everlast PP60S plasma
    thermal arc 250 GTS inverter
    2016 Everlast 250EX
    miller tig cooler
    2015 Everlast MTS250S
    Miller 30A spool Gun
    Miller xtreme 12VS wire feeder
    Linde CM 85 shape cutter

  3. #3
    Join Date
    Oct 2010
    Location
    Northern Virginia
    Posts
    1,323

    Default

    Got ya- thanks!
    DaveO
    Oxweld oxy acet gear
    IMIG 200
    PowerTIG 210 EXT... Amazing!

  4. Default

    To be clear even a piece of alum. that had the oxide coating cleaned off of it one day should be cleaned again if the welding on it is not completed within the same day . I personally would not clean it again unless it was a critical part that needs top strength, like an airplane part .
    Miller 302 gas drive
    millermatic 200 mig
    miller spoolmatic 3 spool gun with 100ft ext.
    2014 Everlast PP60S plasma
    thermal arc 250 GTS inverter
    2016 Everlast 250EX
    miller tig cooler
    2015 Everlast MTS250S
    Miller 30A spool Gun
    Miller xtreme 12VS wire feeder
    Linde CM 85 shape cutter

  5. #5

    Default

    I tig a ton of aluminum. Use an Everlast 250 EX.

    I use a wire wheel which is only used for aluminum and wire wheel the areas I am about to weld. I then use a product called Arcare Protex Aluminum Cleaner. I just pour a little on and spread it around with a small rag. I then let it dry. It keeps the aluminum from oxidizing. When I am ready to weld, I use a bit of Acetone to clean it up and I also use a bit of Acetone on a rag and run my aluminum tig rods through it. You will be surprised at how dirty those rods are!

    After cleaning all that up like that, you will get sparkling clean tig welds that have no black soot in them at all.
    Powertig 250EX
    Powerplasma 50
    Hobart Handler 210 with spoolgun
    Cobra 2000 / Henrob O/A torch
    Drill press / metal brake / 36 ton air hydraulic press
    Franzinated modified Craftsman 33 compressor
    Lots of other metal working tools

Similar Threads

  1. aluminum welding with mig
    By rebelbah in forum MIG Welding (GMAW/GMAW-P/FCAW)
    Replies: 2
    Last Post: 10-18-2016, 04:36 PM
  2. mig welding aluminum
    By Rodsmachineshop in forum MIG Welding (GMAW/GMAW-P/FCAW)
    Replies: 3
    Last Post: 06-20-2012, 11:50 AM
  3. tig welding aluminum with a DC only tig
    By rab in forum General Welder Questions
    Replies: 18
    Last Post: 04-03-2012, 02:25 AM
  4. Replies: 2
    Last Post: 08-03-2011, 03:50 PM
  5. Tig welding aluminum
    By Tallguy64 in forum General Welding Questions
    Replies: 6
    Last Post: 04-10-2010, 11:02 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •